Table 1 Optical properties of single VO2 samples and spinodal decomposition samples.
From: Multi-nanolayered VO2/Sapphire Thin Film via Spinodal Decomposition
Sample | T lum (%) | T sol (%) | ΔT sol (%) | ΔT 2000nm (%) | T c-heating (°C) | T c-cooling (°C) | ΔT c (°C) | ||
---|---|---|---|---|---|---|---|---|---|
20 °C | 90 °C | 20 °C | 90 °C | ||||||
V-A | 40.7 | 40.0 | 40.5 | 34.4 | 6.1 | 46.4 | 57.6 | 52.8 | 4.8 |
SD-A | 42.7 | 39.7 | 45.4 | 35.8 | 9.6 | 51.7 | 50.6 | 47.0 | 3.6 |
V-R | 39.8 | 38.7 | 39.6 | 33.0 | 6.6 | 43.7 | 52.7 | 45.3 | 7.4 |
SD-R | 22.7 | 29.1 | 38.8 | 34.1 | 4.7 | 50.5 | 51.6 | 47.5 | 4.1 |
V-C | 41.1 | 40.7 | 43.3 | 35.8 | 7.5 | 45.0 | 55.8 | 50.7 | 5.1 |
SD-C | 41.5 | 42.1 | 48.6 | 45.3 | 3.3 | 17.6 | 67.1 | 61.1 | 6.0 |
V-M | 45.0 | 41.8 | 44.5 | 36.5 | 8.0 | 52.5 | 55.6 | 48.8 | 6.8 |