Table 2 Photovoltaic performance parameters of fresh and aged devices under ISOS-D-3 and ISOS-T-3 degradation conditions.
From: Degradation pathways in standard and inverted DBP-C70 based organic solar cells
Devices | VOC (V) | JSC (mA/cm2) | PCE (%) | FF (%) |
---|---|---|---|---|
St-Fresh | 0.85 ± 0.05 | 5.8 ± 0.26 | 3.50 ± 0.17 | 71.2 ± 1.1 |
In-Fresh | 0.72 ± 0.07 | 5.88 ± 0.57 | 2.68 ± 0.29 | 62.0 ± 2.5 |
St-ISOS-D-3 | 0.36 ± 0.28 | 4.90 ± 1.44 | 0.68 ± 0.73 | 23.3 ± 16.7 |
In-ISOS-D-3 | 0.03 ± 0.05 | 5.60 ± 0.54 | 0.01 ± 0.02 | 7.3 ± 14.5 |
St-ISOS-T-3 | 0.87 ± 0.05 | 5.67 ± 0.34 | 2.94 ± 0.52 | 59.3 ± 6.7 |
In-ISOS-T-3 | 0.45 ± 0.07 | 5.86 ± 0.93 | 1.02 ± 0.55 | 37.9 ± 13.8 |