Table 4 Summary of compressive properties of PAAm-MSiO2 hydrogels prepared by varying the concentration of AAm (3 M, 4 M, and 5 M) and keeping the constant concentration (0.75 wt%) of MSiO2 particles having different diameters (117.5 nm, 216.5 nm, and 311.5 nm).

From: Effect of sizes of vinyl modified narrow-dispersed silica cross-linker on the mechanical properties of acrylamide based hydrogel

Hydrogel code

Young’s modulus (kPa)

Compressive strength (kPa)

Toughness (kJ/m3)

117.5 nm MSiO2

216.5 nm MSiO2

311.5 nm MSiO2

117.5 nm MSiO2

216.5 nm MSiO2

311.5 nm MSiO2

117.5 nm MSiO2

216.5 nm MSiO2

311.5 nm MSiO2

PAAm (3 M)-MSiO2 0.75% hydrogel

0.11

0.10

0.19

18

26

34

3.5

4.0

6.0

PAAm (4 M)-MSiO2 0.75% hydrogel

0.15

0.18

0.27

26

44

46

5.2

9.0

9.0

PAAm (5 M)-MSiO2 0.75% hydrogel

0.25

0.27

0.41

43

49

78

8.9

10.0

16.0