Table 3 Coating formulation of high gloss paint and preparation steps.

From: Preparation of new surface coating based on modified oil-based polymers blended with ZnO and CuZnO NPs for steel protection

Prepared nanocomposite alkyd/or nanocomposite polyester amide resin

50

Xylene

5

Stirring 3 min. for good mixing

 Anti-settling gel

3

Stirring for 5 min. for completely miscible

F umed silica

0.5

Stirring for 5 min. for completely soluble

 Anti-terra U

1

 Titanium dioxide

20

 Talk powder

15

 Xylene

7

 CaCO3

6

High speed until reach to optimum fineness (be careful, Temperature should be up to 45 °C

Low speed for the following

 Prepared nanocomposite alkyd/or nanocomposite polyester amide resin

30

 Dryers

0.5

 Xylene

4

 Iso-butanol

2.5

 Methyl ethyl ketoxime

03

 UV. stabilizer

0.1