Table 5 Response surface experimental design and results.

From: Optimizing fluidity and tensile strength of magnetically driven epoxy-cement repair materials based on response surface

Standard order

Factor

Tensile strength (MPa)

Fluidity (mm)

ER content (%)

Water-cement ratio

Fe3O4 content (%)

SAC content (%)

1

5

0.45

10

2.5

1.87

245.00

2

9

0.45

10

2.5

2.57

226.00

3

5

0.55

10

2.5

0.82

266.00

4

9

0.55

10

2.5

1.43

255.00

5

5

0.45

20

2.5

1.85

238.00

6

9

0.45

20

2.5

1.65

216.00

7

5

0.55

20

2.5

1.33

264.00

8

9

0.55

20

2.5

1.26

244.00

9

5

0.45

10

7.5

1.21

233.00

10

9

0.45

10

7.5

1.78

221.00

11

5

0.55

10

7.5

0.98

243.00

12

9

0.55

10

7.5

1.63

248.00

13

5

0.45

20

7.5

1.12

233.00

14

9

0.45

20

7.5

1.31

217.00

15

5

0.55

20

7.5

1.57

255.00

16

9

0.55

20

7.5

2.03

242.00

17

3

0.5

15

5

1.01

255.00

18

11

0.5

15

5

1.98

209.00

19

7

0.4

15

5

1.86

204.00

20

7

0.6

15

5

1.14

259.00

21

7

0.5

5

5

1.66

247.00

22

7

0.5

25

5

1.93

229.00

23

7

0.5

15

0

1.34

243.00

24

7

0.5

15

10

1.37

228.00

25

7

0.5

15

5

2.05

235.00

26

7

0.5

15

5

1.98

235.00

27

7

0.5

15

5

2.18

235.00

28

7

0.5

15

5

2.12

235.00

29

7

0.5

15

5

2.09

235.00

30

7

0.5

15

5

2.18

235.00