Table 2 Laboratory test conditions.

From: Thiosulfate leaching in carbonaceous gold-bearing ores in Ethiopia

No

Experimental conditions

First run

Second run

1

Head grade

1.25 g/t

1.25 g/t

2

Sodium cyanide (NaCN) strength

0.5 g/l

0.25 g/l

3

Sodium thiosulfate (Na2S2O3) strength

9 g/l

8 g/l

4

Ammonia (NH3)

13.6 g/l

13.6 g/l

5

Copper sulfate (CuSO4)

0.8 g/l

0.8 g/l

6

Sample size

2 kg

2 kg

7

Pulp density

50% Solid

50% Solid

8

pH

10.0

11.5

9

Leaching time

48 h

48 h

10

Temperature

20–25 °C (Room temp.)

20–25 °C (Room temp.)