Table 4 The compressive strength values for various specimens cured at 7 bar/178oC.

From: Recycling some byproducts for fabrication of green cement with good mechanical strength and high efficiency for wastewater treatment

Time of autoclaving (hr)

Compressive strength (MPa)

C

C-20B

C-30B

C-10B10S

C-20B10S

1

56.7

36.3

31.4

60.3

52.2

4

80.0

54.2

45.4

72.6

63.7

8

83.3

60.6

47.1

75.0

69.6

12

92.8

71.2

51.0

78.7

72.4