Table 12 Normalized concentrations, mass loss, and glass dissolution rates for si, B, U, ce, nd, and Eu in the lanthanide and uranium loaded borosilicate glass sample series were evaluated during the PCT-B test from days 3 to 10.
From: Structural characterization of uranium and lanthanide loaded borosilicate glass matrix
 | REF 3D | REF 7D | REF 10D | MUCe 3D | MUCe 7D | MUCe 10D | MUNd 3D | MUNd 7D | MUNd 10D | MUEu 3D | MUEu 7D | MUEu 10D | MUCNE 3D | MUCNE 7D | MUCNE 10D |
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
NC(Si) [g/L] | 0.686 | 1.516 | 1.787 | 1.863 | 6.491 | 9.536 | 7.292 | 13.03 | 25.67 | 0.135 | 15.17 | 17.60 | 0.182 | 0.164 | 0.146 |
f(Si) - | 0.222 | 0.222 | 0.222 | 0.156 | 0.156 | 0.156 | 0.156 | 0.156 | 0.156 | 0.156 | 0.156 | 0.156 | 0.134 | 0.134 | 0.134 |
NL(Si) [g/m2] | 0.43 | 0.94 | 1.11 | 1.15 | 4.06 | 5.94 | 4.535 | 8.129 | 16.08 | 0.084 | 9.446 | 10.97 | 0.113 | 0.102 | 0.091 |
NR(Si) [g/(m2d)] | 0.142 | 0.134 | 0.111 | 0.385 | 0.580 | 0.594 | 1.512 | 1.161 | 1.608 | 0.028 | 1.349 | 1.097 | 0.038 | 0.015 | 0.009 |
NC(B) [g/L] | 1.400 | 2.424 | 2.592 | 1.897 | 5.220 | 7.628 | 8.679 | 17.73 | 25.51 | 1.078 | 8.938 | 11.64 | 0.339 | 0.405 | 0.449 |
f(B) - | 0.032 | 0.032 | 0.032 | 0.022 | 0.022 | 0.022 | 0.022 | 0.022 | 0.022 | 0.022 | 0.022 | 0.022 | 0.019 | 0.019 | 0.019 |
NL(B) [g/m2] | 0.87 | 1.50 | 1.61 | 1.176 | 3.264 | 4.755 | 5.398 | 11.06 | 15.98 | 0.671 | 5.57 | 7.25 | 0.210 | 0.252 | 0.279 |
NR(B) [g/(m2d)] | 0.29 | 0.214 | 0.161 | 0.392 | 0.466 | 0.475 | 1.799 | 1.580 | 1.598 | 0.224 | 0.795 | 0.725 | 0.070 | 0.036 | 0.028 |
NC(U) [g/L] | - | - | - | 1.41E-04 | 1.70E-03 | 3.21E-03 | 2.65E-03 | 8.18E-03 | 2.16E-02 | 1.29E-04 | 2.39E-03 | 2.49E-03 | 1.47E-04 | 1.23E-04 | 1.72E-04 |
f(U) - | - | - | - | 0.166 | 0.166 | 0.166 | 0.166 | 0.166 | 0.166 | 0.166 | 0.166 | 0.166 | 0.083 | 0.083 | 0.083 |
NL(U) [g/m2] | - | - | - | 8.76E-05 | 1.06E-03 | 2.00E-03 | 1.65E-03 | 5.10E-03 | 1.35E-02 | 8.03E-05 | 1.49E-03 | 1.55E-03 | 9.16E-05 | 7.65E-05 | 1.07E-04 |
NR(U) [g/(m2d)] | - | - | - | 2.92E-05 | 1.51E-04 | 2.00E-04 | 5.50E-04 | 7.29E-04 | 1.35E-03 | 2.68E-05 | 2.13E-04 | 1.55E-04 | 3.05E-05 | 1.09E-05 | 1.07E-05 |
NC(Ce) [g/L] | - | - | - | < LOD | 5.33E-05 | 3.64E-05 | - | - | - | - | - | - | 3.11E-05 | 3.93E-05 | 9.10E-06 |
f(Ce) - | - | - | - | 0.081 | 0.081 | 0.081 | - | - | - | - | - | - | 0.081 | 0.081 | 0.081 |
NL(Ce) [g/m2] | - | - | - | - | 3.33E-05 | 2.27E-05 | - | - | - | - | - | - | 1.93E-05 | 2.45E-05 | 5.65E-06 |
NR(Ce) [g/(m2d)] | - | - | - | - | 4.76E-06 | 2.27E-06 | - | - | - | - | - | - | Â | Â | Â |
NC(Nd) [g/L] | - | - | - | - | - | - | 2.88E-05 | 5.42E-05 | 9.37E-05 | - | - | - | < LOD | < LOD | < LOD |
f(Nd) - | - | - | - | - | - | - | 0.086 | 0.086 | 0.086 | - | - | - | 0.086 | 0.086 | 0.086 |
NL(Nd) [g/m2] | - | - | - | - | - | - | 1.79E-05 | 3.38E-05 | 5.87E-05 | - | - | - | - | - | - |
NR(Nd) [g/(m2d)] | - | - | - | - | - | - | 5.97E-06 | 4.83E-06 | 5.87E-06 | - | - | - | - | - | - |
NC(Eu) [g/L] | - | - | - | - | - | - | - | - | - | 1.98E-06 | 2.11E-05 | < LOD | 4.11E-06 | < LOD | 1.69E-06 |
f(Eu) - | - | - | - | - | - | - | - | - | - | 0.086 | 0.086 | 0.086 | 0.086 | 0.086 | 0.086 |
NL(Eu) [g/m2] | - | - | - | - | - | - | - | - | - | 1.23E-06 | 1.31E-05 | - | 2.55E-06 | - | 1.05E-06 |
NR(Eu) [g/(m2d)] | - | - | - | - | - | - | - | - | - | 4.11E-07 | 1.87E-06 | - | 8.51E-07 | - | 1.05E-07 |