Table 5 EIS parameters for painted steel at different concentrations of the synthesized nanocomposite in 3.5% NaCl solution.

From: Enhancing corrosion resistance with chemically modified aluminum oxide in UV-curable coatings applied to steel surfaces

Conc.a

(wt%)

RS

(Ω cm2)

Cdl

(µF cm2) 106

Rct

(kΩ cm2)

CPEct

Rf

(kΩ cm2)

CPEf

Rp

(kΩ cm2)

(%)

Y0

(μΩsncm-2) 10–5

n

Y0

(μΩsncm-2)

10–7

n

value

Standard deviation × 10–2

Blank

10.15

447.00

0.428

59.72

0.78

0.198

  

0.626

1.050397

0

10.53

123.11

0.532

7.458

0.68

25.132

1325

0.38

25.664

17.40412

98.7

2

12.78

18.22

0.629

1.872

0.80

33.105

2.923

0.80

33.734

63.49622

98.9

4

11.65

2.31

61.615

0.4687

0.48

41.818

8.034

0.61

103.433

115.9023

99.5

6

13.55

1.45

152.742

0.2037

0.61

49.862

9.825

0.67

202.604

153.2155

99.8

8

14.84

0.91

234.324

0.1631

0.55

54.405

3.260

0.69

288.729

101.4889

99.9

  1. a= Conc. of nAl2O3-Silane in polymer matrix