Table 1 Synthesis conditions of nanohybrids
Methods | Nanoparticles | Size nm | Metal salts mM (mmol/L) | NaBH4 mM | Stabilizers mM | Reaction Temperature (T) °C | Receiver T °C | Flow rate mL/min |
---|---|---|---|---|---|---|---|---|
All NMP-phased reaction systems | FeAl@Al(1-x)FexOy | 4.8 ± 0.3 | FeCl2·4H2O: 27; AlCl3: 12 | 120 | PVP: 0.94 | 80 | 10 | 1.0 |
 | CoZn@Zn(1-x)CoxOy | 3.5 ± 0.3 | CoCl2·6H2O: 32; ZnCl2: 120 | 1016 | PVP: 0.84 | 80 | 10 | 0.8 |
Aqueous-phased metal-salt reaction systems | CoZn@Zn(1-x)CoxOy | 4.4 ± 0.4 | CoCl2·6H2O: 10; ZnCl2: 3 | 175 | PVP: 0.7; VC: 5.5 | 80 | 10 | 3.0 |
 | AuZn@Zn(1-x)AuxOy | 3.6 ± 0.2 | HAuCl4·xH2O: 29; ZnCl2: 50 | 180 | PVP: 0.92 | 80 | 10 | 3.0 |
 | AgAl@Al(1-x)AgxOy | 3.7 ± 0.3 | AgNO3: 25; AlCl3: 10 | 175 | PVP: 0.46 | 80 | 10 | 5.0 |