Table 1 The composition used for preparing the composite.

From: Preparation and application of conducting polymer/Ag/clay composite nanoparticles formed by in situ UV-induced dispersion polymerization

Sample

ATP (g)

Pyrrole (mL)

ATP/pyrrole a

AgNO 3 b(g)

Size of Ag (nm)

Conductivity (S/cm)

S-1

0.048

1.0

5:100

2.45

33

S-2

0.097

1.0

10:100

2.45

37

0.122

S-3

0.193

1.0

20:100

2.45

40

0.442

S-4

0.290

1.0

30:100

2.45

38

0.299

S-5

0.484

1.0

50:100

2.45

37

0.340

  1. amass ratio; b fixed 1:1 molar ratio of AgNO3 to pyrrole.