Table 1 Summary of WVTR and rate of change of wrinkle encapsulation before and after bending at different preparation temperatures

From: Innovative stress-release method for low-stress flexible Al2O3 encapsulation films in OLED applications

Temperature (°C)

Bending radius (mm)

Bending repetitions(times)

Test condition (°C/% RH)

Before bending WVTR (g/m2/day)

After bending WVTR (g/m2/day)

Rate of change (%)

RT

2

10,000

60/90

4.49 × 10−5

4.96 × 10−5

10.4%

35

2

10,000

60/90

3.44 × 10−5

3.61 × 10−5

5.0%

40

2

10,000

60/90

2.82 × 10−5

3.01 × 10−5

6.7%

45

2

10,000

60/90

2.35 × 10−5

2.51 × 10−5

6.8%

50

2

10,000

60/90

1.05 × 10−5

1.13 × 10−5

7.6%