Table 4 Delayed descriptive statistics for µSBS (MPa).

From: Immediate and delayed micro shear bond strength evaluation of two glass ionomer cements to composite resin by using different bonding techniques—an in vitro study

Material

Finishing stone grit

Conditioning

Mean

95% CI

SD

Min.

Max.

Lower

Upper

Riva LC

Smooth

SE

14.48

11.78

17.18

4.36

8.70

21.79

TE

18.31

14.96

21.66

5.40

11.50

27.73

Medium

SE

14.59

12.23

16.96

3.81

9.40

20.55

TE

18.78

15.81

21.75

4.79

8.58

25.00

Rough

SE

12.40

10.23

14.56

3.50

8.18

17.56

TE

15.28

13.40

17.17

3.04

9.80

18.70

Riva SC

Smooth

SE

8.26

6.55

9.96

2.75

3.00

11.30

TE

6.54

5.65

7.43

1.44

4.30

8.25

Medium

SE

10.66

8.94

12.38

2.77

6.00

14.20

TE

10.47

9.47

11.47

1.61

7.22

12.77

Rough

SE

7.72

6.14

9.29

2.54

4.70

12.44

TE

11.20

8.29

14.10

4.68

2.10

18.84

  1. SD standard deviation
  2. 95%CI = 95% confidence interval for the mean