Table 2 Determined chloride deposition densities, segmented crack length, and estimated crack growth

From: Time-dependent in situ measurement of atmospheric corrosion rates of duplex stainless steel wires

Sample

Applied load

Strain

Mean chloride deposition density

Mean corrosion rate

Max. crack length

Mean crack growth rate

Exposure (days)

(MPa)

(µm/year)

(µm)

(µm/year)

2202–1

700

Yield (YS)

44 µg/cm²

8

≈80b

55

542

2205–2

550

65% Yield

88 µg/cm²

7

≈100a

53

676

2205–3

900

120% Yield

58 µg/cm²

5

≈100b

69

615

2205–4

930

1% Strain

63 µg/cm²

6

>1000b

>690

524

  1. aDetermined by X-ray CT
  2. bDetermined by SEM. Crack length determined by X-ray CT are in depth whereas those determined by SEM are superficial