Table 3 Dielectric constant and dielectric loss of Ba0.6Sr0.4TiO3/PVdF-HFP nanocomposite synthesized by fluorination and sonication at a frequency of 1 MHz.

From: Tunable Dielectric Properties of Poly(vinylidenefluoride-co-hexafluoropropylene) Films with Embedded Fluorinated Barium Strontium Titanate Nanoparticles

Nanocomposite

Fluorination

Sonication

Dielectric constant

Dielectric loss

AFM image

Ba0.6Sr0.4TiO3/PVdF-HFP

X

X

2 (±1.9)

11 (±8)

Fig. S5(a)

X

O

2 (±1.5)

10 (±5)

Fig. S5(b)

Fluorinated Ba0.6Sr0.4TiO3/PVdF-HFP

O

X

18.5 (±1.8)

0.024 (±0.08)

 

O

O

18.4 (±1.7)

0.023 (±0.05)

Fig. 3(c)