Table 1 Comparison of relative density and electrical conductivity of various Ti3AlC2 and TiC ceramics.
Sample | Preparation Conditions | Relative Density | Electrical Conductivity |
|---|---|---|---|
TAC-A | Pressureless sintering (1500 °C, 2 h) | 91.2% | 2.4*106 S/m |
TAC-B | Hot-pressing (1350 °C, 15 min) | 95.6% | 2.9*106 S/m |
TAC-C | Hot-pressing (1400 °C, 2 h) | 98.5% | 3.0*106 S/m |
TAC-D | Hot-pressing (1400 °C,2 h) + Pressureless sintering (1500 °C, 10 h) | 98.2% | 3.2*106 S/m |
TiC-A | Hot-pressing (1800 °C, 15 min) | 98.6% | 4.2*106 S/m |
TiC-B | Hot-pressing (1950 °C, 2 h) | 98.9% | 4.7*106 S/m |