Table 1 Mechanical properties of all the wet-spun fibres with the standard deviation.
From: Graphene oxide incorporated waste wool/PAN hybrid fibres
Sample | Diameter (µm) | Linear density (tex) | Strength (MPa) | Strain (%) |
|---|---|---|---|---|
Control PAN | 16.96 ± 1.74 | 0.16 ± 0.01 | 438.32 ± 1.96 | 8.66 ± 0.76 |
WP (5:95) | 19.84 ± 1.41 | 0.18 ± 0.02 | 342.83 ± 2.53 | 11.37 ± 0.68 |
WP (15:85) | 23.42 ± 2.05 | 0.24 ± 0.02 | 192.12 ± 1.78 | 11.62 ± 1.41 |
WP (25:75) | 30.39 ± 2.40 | 0.33 ± 0.02 | 116.67 ± 1.95 | 12.07 ± 1.75 |
WP (25:75)a | 20.58 ± 1.60 | 0.19 ± 0.02 | 327.28 ± 1.98 | 10.92 ± 1.39 |