Table 3 Experimental parameters and CTOD value.

From: Mechanical, microstructural and fracture studies on inconel 825–SS316L functionally graded wall fabricated by wire arc additive manufacturing

Sample geometry

SENB

SENB

Notch side

Inconel 825

SS316L

Orientation

L–T

L–T

Thickness (B) mm

10.24

10.20

Width (W) mm

20.02

20.06

Notch length (a0) mm

7.00

7.00

Terminal pre-cracking force (Pf) kN

2.66

2.34

Number of cycles

39,684

36,802

Final crack length (a) mm

9.43

9.67

Maximum load value at fracture (Pmax) kN

5.37

4.55

Crack tip opening displacement (CTOD) mm

0.853

0.873

Fracture toughness (KIC)

36 Mpa\(\sqrt {\mathbf{m}}\)

31.6 Mpa\(\sqrt {\mathbf{m}}\)

  1. Significant values are in bold.