Table 2 Crystallite size values determined by scherrer and Williamson-Hall method for the Zn1−xCoxO nrs.

From: An investigation on structural, optical, and magnetic properties of Zn1−xCoxO nanorods fabricated by electrochemical deposition

Samples

XRD Peak

Angle (2\(\:\varvec{\theta\:})\)

Scherrer method

Williamson-hall method

Crystallite size (D) (nm)

Average crystallite size (nm)

Crystallite size (D) (nm)

Strain

S0

(010)

31.478

48.57

57.10

-

-

(002)

34.149

73.57

(011)

35.963

49.15

S1

(010)

31.505

27.52

27.70

-

-

(002)

34.143

24.74

(011)

35.994

30.83

S2

(010)

31.419

28.47

25.75

66.3

0.00289

(002)

34.077

21.81

(011)

35.920

26.95

S3

(010)

31.430

25.80

25.48

30.1

0.000713

(002)

34.095

25.34

(011)

35.922

25.31