Table 3 Mix properties of concretes (kg/m3).

From: Performance and statistical characteristics of ferronickel slag geopolymer concrete

No

Specimen

FA

GBFS

Stone

NS

FNS

NaOH

Water glass

Water

Superplasticizer

1

AB3-WB0.45–0

153

358

920

614

0

27

139

134

8

2

AB3-WB0.45–33

153

358

920

411

203

27

139

134

8

3

AB3-WB0.45–66

153

358

920

203

411

27

139

134

8

4

AB3-WB0.45–100

153

358

920

0

614

27

139

134

8

5

AB5-WB0.45–0

107

249

1068

712

0

19

97

93

5

6

AB5-WB0.45–33

107

249

1068

477

235

19

97

93

5

7

AB5-WB0.45–66

107

249

1068

235

477

19

97

93

5

8

AB5-WB0.45–100

107

249

1068

0

712

19

97

93

5

9

AB4-WB0.4–0

127

296

1016

677

0

22

115

90

6

10

AB4-WB0.4–33

127

296

1016

454

223

22

115

90

6

11

AB4-WB0.4–66

127

296

1016

233

454

22

115

90

6

12

AB4-WB0.4–100

127

296

1016

0

677

22

115

90

6

13

AB4-WB0.5–0

125

291

998

665

0

22

113

130

6

14

AB4-WB0.5–33

125

291

998

446

219

22

113

130

6

15

AB4-WB0.5–66

125

291

998

219

446

22

113

130

6

16

AB4-WB0.5–100

125

291

998

0

665

22

113

130

6