Table 7 Tensile strength parallel to the grain of thermally modified wood of Salix tetrasperma (kN/mm2).
From: Enhanced strength and chemical stability of Salix tetrasperma wood through thermal modification
Duration(h) Temperature (°C) | 2 h | 4 h | 6 h | Mean | SD | CV |
|---|---|---|---|---|---|---|
60 °C | 0.049 | 0.049 | 0.047 | 0.049 | 0.0012 | 2.3890 |
80 °C | 0.048 | 0.056 | 0.047 | 0.050 | 0.0049 | 9.8004 |
100 °C | 0.053 | 0.055 | 0.054 | 0.054 | 0.0010 | 1.8519 |
120 °C | 0.070 | 0.059 | 0.047 | 0.059 | 0.0115 | 19.6084 |
140 °C | 0.048 | 0.049 | 0.047 | 0.048 | 0.0010 | 2.0833 |
160 °C | 0.048 | 0.045 | 0.040 | 0.044 | 0.0040 | 9.1161 |
180 °C | 0.046 | 0.042 | 0.044 | 0.044 | 0.0020 | 4.5455 |
200 °C | 0.041 | 0.042 | 0.038 | 0.040 | 0.0021 | 5.1612 |
Control | 0.049 | 0.049 | 0.049 | 0.049 | ||
Mean | 0.050 | 0.049 | 0.046 |
CD0.05 | |
|---|---|
Temperature (T) | 0.003 |
Duration (D) | 0.002 |
Temperature × Duration (T × D) | 0.006 |