Table 11 Structural parameters of soot samples from XRPD
From: The reproduction of fire-born soot for comparative cleaning tests on heritage objects
Sample | Xc (%) | (002) peak | K = 0.89 | (100) peak | K = 1.84 | ||||
|---|---|---|---|---|---|---|---|---|---|
2ϑ (o) | FWHM | d002 (Å) | Lc (Å) | 2ϑ (o) | FWHM | d100 (Å) | La (Å) | ||
lamp black_NP | 86.925 | 24.479 | 5.757 | 2.399 | 14.409 | 43.576 | 3.816 | 3.818 | 43.456 |
furnace black_Kr | 85.157 | 24.364 | 5.525 | 2.055 | 15.338 | 43.558 | 3.803 | 3.661 | 43.685 |
carbon black_NP | 81.585 | 24.350 | 5.318 | 2.019 | 15.981 | 43.750 | 3.518 | 6.647 | 46.480 |
candle soot | 53.886 | 24 (LDCC) | 6.810 | 1.436 | 13.671 | / | |||
26 (MDCC) | 9.111 | 1.833 | 9.502 | ||||||
drum soot | 51.662 | 24.650 | 5.231 | 3.223 | 15.466 | / | |||