Table 1 Shear properties of monolayer Ti3C2Tx under in-plane shear loading
From: Shear properties and stable wrinkle resistance in 2D Ti3C2Tx MXene monolayers
Sample # | Width b (μm) | Length W (μm) | Shear modulus \({G}_{3D}^{{Stage}1}\) (GPa) | Shear modulus \({G}_{3D}^{{Stage}3}\) (GPa) | Fracture strain γ (%) | Fracture strength τ (GPa) |
|---|---|---|---|---|---|---|
1 | 5.5 | 4.5 | 274.1 | 103.8 | 8.9 | 17.2 |
2 | 5.5 | 4.5 | 284.9 | 117.3 | 8.7 | 19.3 |
3 | 5.5 | 4.5 | 276.5 | 114.0 | 8.2 | 19.9 |
4 | 5.5 | 4.5 | 279.8 | 107.5 | 8.7 | 17.9 |
Average | 278.8 ± 7.4 | 110.7 ± 9.7 | 8.6 ± 0.5 | 18.6 ± 2.0 |