Table 1 Summary of GFRP bar-UPC pull-out bond test results.

From: Durability assessment of the bonding performance between GFRP rebars and UPC in aquatic environments

Specimen number

Maximum bond force

Average maximum bond force

Bond strength

Average bond strength

Fmax (kN)

\(\overline{F}_{{{\text{max}}}}\) (kN)

τmax (MPa)

\(\overline{\tau }_{{{\text{max}}}}\) (MPa)

 

49.50

 

31.53

 

control

47.25

48.30

30.10

30.76

 

48.15

 

30.67

 
 

50.25

 

32.01

 

T25-60d

48.75

49.40

31.05

31.47

 

49.2

 

31.34

 
 

47.25

 

30.1

 

T25-120d

48.05

47.38

30.61

30.18

 

46.85

 

29.84

 
 

47.15

 

30.03

 

T25-180d

46.85

46.55

29.84

29.65

 

45.65

 

29.08

 
 

48.75

 

31.05

 

T40-60d

48.25

48.48

30.73

30.88

 

48.45

 

30.86

 
 

47.05

 

29.97

 

T40-120d

46.35

46.50

29.52

29.62

 

46.10

 

29.36

 
 

44.65

 

28.44

 

T40-180d

45.85

45.49

29.20

28.97

 

45.95

 

29.27

 
 

46.95

 

29.9

 

T60-60d

47.15

47.62

30.03

30.33

 

48.75

 

31.05

 
 

46.60

 

29.68

 

T60-120d

45.85

45.73

29.20

29.13

 

44.75

 

28.5

 
 

43.95

 

27.99

 

T60-180d

44.25

44.53

28.14

28.35

 

45.40

 

28.92