Table 4 Measured averaged tensile properties.
From: Tensile properties of the neutron irradiated HT-9 ACO-3 duct
Condition | Ttest | YS (MPa) | UTS (MPa) | ε uniform (%) | ε total (%) |
|---|---|---|---|---|---|
6 E 9 | RT | 1032 | 1072 | 2.1 | 10.0 |
382 °C, 22 dpa | 200 | 912 | 940 | 1.5 | 9.4 |
350 | 874 | 893 | 1.3 | 8.0 | |
6 E 5 | RT | 974 | 1034 | 2.3 | 10.1 |
399 °C, 42 dpa | 200 | 901 | 937 | 1.7 | 9.7 |
400 | 799 | 840 | 1.4 | 8.8 | |
6 E 1 | RT | 879 | 969 | 3.2 | 11.4 |
416 °C, 110 dpa | 200 | 774 | 853 | 2.4 | 7.8 |
400 | 702 | 770 | 2.3 | 8.7 | |
5 E 1 | RT | 665 | 847 | 7.2 | 16.6 |
441 °C, 147 dpa | 200 | 605 | 736 | 5.4 | 13.4 |
450 | 514 | 618 | 4.9 | 13.7 | |
4 E 1 | RT | 558 | 808 | 8.3 | 17.7 |
466 °C, 93 dpa | 200 | 487 | 685 | 6.9 | 15.1 |
450 | 400 | 549 | 5.6 | 15.5 | |
2 E 1 | RT | 629 | 805 | 5.5 | 13.9 |
504 °C, 3 dpa | 200 | 552 | 699 | 4.6 | 12.7 |
500 | 439 | 509 | 2.7 | 18.9 | |
Control | RT | 551 | 706 | 6.8 | 17.6 |
200 | 528 | 665 | 5.1 | 15.1 | |
350 | 528 | 665 | 5.1 | 15.1 | |
400 | 517 | 648 | 4.6 | 13.3 | |
450 | 488 | 603 | 4.2 | 15.2 | |
500 | 458 | 544 | 4.1 | 22.8 |