Table 4 Summary of the phase transformation temperatures of alloy 718 + TiB2 registered by DSC.

From: Microstructure, phase transformation temperatures and long-term stability of ex-situ Alloy 718 + TiB2 metal-ceramic nanocomposites as a repair coatings for aerospace applications

Addition of TiB2 to Alloy 718, wt%

0

1.25

2.5

3.75

5.0

 

Upon heating at 20 °C/min 

Max. rate of Laves phase dissolution, °C

1186

1130

1129

1131

1139

Max. rate of B-rich phases dissolution, °C

1212

1215

1216

1214

Liquidus, °C

1362

1332

1291

1251

1214

 

Upon cooling at 20 °C/min

Liquidus, °C

1344

1308

1279

1238

1200

Solidus, °C

1244

1116

1087

1098

1080

Max. rate of Laves/B-rich phases precipitation, °C

1156

1158

1159

1166/1150

1174/1144