Table 6 Double shear test results.

From: Fatigue characteristics and mechanical evaluation of basalt fiber reinforced composite material concrete under freeze-thaw cycles

Specimen number

Concrete strength grade

Bond thickness/mm

Bond length/mm

Bond width/mm

Freeze-thaw cycles/cycle

Ultimate load/kN

JL-0

C40

1

120

50

0

28.38

JL-100

C40

1

120

50

100

25.93

JL-200

C40

1

120

50

200

23.36

Specimen number

Maximum fatigue load (Pmax)/kN

Minimum fatigue load(Pmin)/kN

Fatigue load amplitude (ΔP)/kN

Fatigue life (N)/cycles

PL-0

19.87

18.15

16.35

3.97

15.90

14.52

13.08

18,893

PL-100

3.63

16,109

PL-200

3.27

13,547